Chapter 16 Stainless Steels -
Machining Data
[
Back ] [ Home ] [
Up ] [ Table of Contents ] [ Next ]
FACE MILLING DATA FOR
AUSTENITIC STAINLESS STEELS
|
|
Hardness HB |
|
High Speed Steel Tool |
Coated Carbide Tool |
|
Material |
Heat |
Cut |
Speed |
Feed per |
Tool |
Speed |
Feed per |
Tool |
|
AISI |
Treatmenta |
Depth in |
fpm |
Tooth in |
Material |
fpm |
Tooth in |
Materialb |
| 201, 202 |
135-185 |
0.040 |
130 |
0.008 |
M2, M7 |
700 |
0.008 |
CC-2 |
| 301, 302, |
A |
0.150 |
100 |
0.012 |
M2, M7 |
475 |
0.012 |
CC-2 |
|
304, 304L, |
|
0.300 |
80 |
0.016 |
M2, M7 |
350 |
0.016 |
CC-2 |
| 308,
321, |
225-275 |
0.040 |
115 |
0.006 |
M2, M7 |
650 |
0.007 |
CC-2 |
| 347,
348 |
CD |
0.150 |
90 |
0.010 |
M2, M7 |
425 |
0.010 |
CC-2 |
| |
|
0.300 |
70 |
0.014 |
M2, M7 |
325 |
0.014 |
CC-2 |
| 302B,
309 |
135-185 |
0.040 |
115 |
0.008 |
M2, M7 |
650 |
0.008 |
CC-2 |
| 309S,
310, |
A |
0.150 |
90 |
0.012 |
M2, M7 |
425 |
0.012 |
CC-2 |
| 316,
316L, |
|
0.300 |
70 |
0.016 |
M2, M7 |
325 |
0.016 |
CC-2 |
| 317,
330 |
225-275 |
0.040 |
100 |
0.006 |
M2, M7 |
525 |
0.007 |
CC-2 |
| |
CD |
0.150 |
75 |
0.010 |
M2, M7 |
400 |
0.010 |
CC-2 |
| |
|
0.300 |
55 |
0.014 |
M2, M7 |
300 |
0.014 |
CC-2 |
| Nitronic
40, |
210-250 |
0.040 |
80 |
0.006 |
M2, M7 |
350 |
0.007 |
CC-2 |
| Nitronic
50, |
A |
0.150 |
60 |
0.010 |
M2, M7 |
275 |
0.010 |
CC-2 |
| Nitrpnic
60 |
|
0.300 |
45 |
0.014 |
M2, M7 |
225 |
0.014 |
CC-2 |
|
a. Heat treatment abbreviations are as follows: A - annealed; CD - cold
drawn. |
| b.
Coated carbide tool material grades are designated by additional prefix
letter C, to distinguish it from the Industry Code system for |
| uncoated
carbide tools. |
|